Installation
Concrete Mix
The concrete mix should be an air entrained mix with a minimum
of 3,000 psi. All concrete should be placed at the same
slump to prevent possible cement shade variations. A 3" to
4" slump is recommended with a 5" maximum. Caution:
Do not use any calcium chloride admixtures.
Application
After the concrete has reached the point where no excess
moisture shows at the surface, but while still plastic
throughout, Dynamicast Color Hardener is applied to the
surface by the
dry-shake method. Water must not be sprinkled or otherwise
added to the surface during application or finishing. The
necessary moisture for the color hardener must come from
the concrete in order to develop proper bond and assure
adequate density for the color-hardened surface. The
first shake should
consume two-thirds of the material, one third being withheld
for the second shake and final touch-up. After the first
shake, the surface is thoroughly floated, either mechanically
or by hand. It should not be troweled between the first
and second shakes. The second shake is then applied evenly
and
the surface floated and troweled. A small quantity of material
should be withheld from the second shake for touching up
non-uniform or weak toned areas as necessary. Long handled
Frescos must not be used. Hand troweling should be minimized
and consistent finishing practices used to insure uniformity
of color.
Maintenance
Properly sealed imprinted concrete may be cleaned with
most commercial cleaning compounds, detergents,
solvents, or mild
alkalis with no adverse effect.
|